Compact Laminate Technical Data and Certifications Material properties tested in accordance to EN 438-2 (average value of production control) - Classification CGS Properties
Norms
Unit
Value
Apparent density
DIN 52350/ISO 1183
g/cm3
≥ 1,4
Thickness (e.g.)
EN 438-2, point 5
mm
10
kg/m2
14,0
Physical data
Weight
Mechanical properties Resistance against stress abrasion
EN 438-2, point 10
U
450
Falling ball impact resistance
EN 438-2, point 21
mm
8
Resistance against scratching
EN 438-2, point 25
Degree
3
Scratch r.
4N
Flexural strength
EN ISO 178
Mpa
100
E-Modulus
EN ISO 178
Mpa
10 000
Tensile strength
EN ISO 527-2
Mpa
60
Susceptibility to cracking
EN 438-2, point 24
5
Thermal properties Dimensional changes during climatic changes, measured at elevated temperatures
EN 438-2, point 17
lenght. %
0,05
cross. %
0,15
Resistance to boiling water
EN 438-2, point 12
%
0,3
Coefficient of thermal expansion
DIN 52328
1/K
20 × 10-6
Thermal conductivity
W/mK
ca. 0,3
Resistance to vapour diffusion
μ
17 200
Surface resistance
DIN 53482
Ohm
109-1011
Resistance to cigarette burns
EN 438-2, point 30
Degree
5 - no visible changes1)
Resistance to hot soucepans
EN 438-2, point 16
Degree
5 - no visible changes, no blisters or cracks2)
MJ/kg
18-20
Level
6-8
Heating value
Optical properties Light fastness
EN 438-2, point 27
1) Slight change in glossy finish, yellow or light brown colours are permitted by EN 438 2) Slight change in glossy finish permitted by EN 438 * These qualities are only suitable for inner lining. The panels should not be exposed to high fluctuations of temperature or moisture. (Recommended range: +15 - +35°C, 30 -70% rel. to air moisture)
Mod. COLAMI Rev. 1 del 10/05/2012
Compact Laminate Technical Data and Certifications Food onta t suitabi ity Regarding the hygiene regulations concerning materials produced to have contact with foodstiffs (D.M. 4/4/85 - G.U. N° 10 Cee 123, 11/05/1983) it is declared that Compact Laminate conforms to the maximum values indicated in Annex IV, Section 2, Paragraph 1. It does not leave free formaldyde in quantities exceeding 0,5 mg/dm2, which is 3 p.p.m., with respect to the real or calculated capacity of the said objet. max 3 p.p.m
for occasional contact
max 0,5 p.p.m
for prolonged occasion
ea tion to ire
assi i ation
Standard Class 2 Europe EN 13501-1 Euroclass
D-s2, d0
Austria A3800/1
Tr1, Q1
Germany DIN 4102
B2
Class 1 Class 1
CSE RF 1/75/A – 3/77
Home Office Italy
Approbation
T0055A10CD100005
Class M1
CSTB
Home Office France
Certification
89.28703A
Class 1
BSI 476 part. 7: 1987
British Standard Institution UK
Certification
49513
Mod. COLAMI Rev. 1 del 10/05/2012
Compact Resistance Technical Data and Certifications Material properties tested in accordance to EN 438-2 (average value of production control) - Classification CGS Properties
Norms
Unit
Value
Apparent density
DIN 52350/ISO 1183
g/cm3
≥ 1,4
Thickness (e.g.)
EN 438-2, point 5
mm
10
kg/m2
14,0
Physical data
Weight
Mechanical properties Resistance against stress abrasion
EN 438-2, point 10
U
450
Falling ball impact resistance
EN 438-2, point 21
mm
8
Resistance against scratching
EN 438-2, point 25
Degree
3
Scratch r.
4N
Flexural strength
EN ISO 178
Mpa
100
E-Modulus
EN ISO 178
Mpa
10 000
Tensile strength
EN ISO 527-2
Mpa
60
Susceptibility to cracking
EN 438-2, point 24
5
Thermal properties Dimensional changes during climatic changes, measured at elevated temperatures
EN 438-2, point 17
lenght. %
0,05
cross. %
0,15
Resistance to boiling water
EN 438-2, point 12
%
0,3
Coefficient of thermal expansion
DIN 52328
1/K
20 × 10-6
Thermal conductivity
W/mK
ca. 0,3
Resistance to vapour diffusion
μ
17 200
Surface resistance
DIN 53482
Ohm
109-1011
Resistance to cigarette burns
EN 438-2, point 30
Degree
5 - no visible changes1)
Resistance to hot soucepans
EN 438-2, point 16
Degree
5 - no visible changes, no blisters or cracks2)
MJ/kg
18-20
Level
6-8
Heating value
Optical properties Light fastness
EN 438-2, point 27
1) Slight change in glossy finish, yellow or light brown colours are permitted by EN 438 2) Slight change in glossy finish permitted by EN 438 * These qualities are only suitable for inner lining. The panels should not be exposed to high fluctuations of temperature or moisture. (Recommended range: +15 - +35°C, 30 -70% rel. to air moisture)
Mod. COREST Rev. 1 del 10/05/2012
Compact Resistance Technical Data and Certifications
Rea tion to fi e
lassifi ation
Standard Class 2 Europe EN 13501-1 Euroclass
D-s2, d0
Austria A3800/1
Tr1, Q1
Germany DIN 4102
B2
Mod. COREST Rev. 1 del 10/05/2012
Compact Exterior Technical Data and Certifications Material properties tested in accordance to EN 438-2 (average value of production control) - Classification CGS Properties
Norms
Unit
Value
EN ISO 1183-1
g/cm3
1,45
Flexural strength
EN ISO 178
Mpa
≥ 90
E-Modulus
EN ISO 178
Mpa
≥ 9500
Tensile strength
EN ISO 527-2
Mpa
≥ 80
DIN 52328
1/K
18 × 10-6
Thermal conductivity
W/mK
0,3
Resistance to vapour diffusion
μ
ca. 17 200
Physical data Apparent density
Mechanical properties
Thermal properties Coefficient of thermal expansion
Artificial weathering
EN ISO 4892-2 3000 h EN 20105-A02 greyscale
4-5
EN ISO 4892-3 1500 h EN 20105-A02 greyscale
4-5
Optical properties UV-light resistance
Reaction to fire classification Europe
EN 13501-1
Switzerland
MA39-VFA Vienna
Euroclass B-s2, d0 for 6-10 mm
EMPA Dübendorf
Fire classification 5.3 for 6 - 10 mm
Germany
DIN 4102
Institute for Construction-Berlin
B1 for 4 - 10 mm
France
NFP 92501
LNE
M1 for 2 - 10 mm
Spain
UNE 23727-90
LICOF
M1 for 6 - 10 mm
Facade permit Germany
Institute for Construction-Berlin
6, 8, 10 mm, Permit-No. Z-33.2-16
ETB guidelines for building components which safeguard against falls, June 1985. Balcony railings.
TU Hannover
Passed (depending on building regulation and railing construction 6, 8 or 10 mm panel thickness)
Avis technique France
CSTB
6, 8, 10 and 13 mm, wood- and metal subconstruction, permit no. AT 2/07-1264, AT 2/07-1265
PERMITS
Mod. COEXTE Rev. 1 del 10/05/2012
Compact Forming Technical Data and Certifications Material properties tested in accordance to EN 438-2 (average value of production control) - Classification CGS Properties
Norms
Unit
Value
Apparent density
DIN 52350/ISO 1183
g/cm3
≥ 1,4
Thickness (e.g.)
EN 438-2, point 5
mm
10
kg/m2
14,0
Physical data
Weight
Mechanical properties Resistance against stress abrasion
EN 438-2, point 10
U
450
Falling ball impact resistance
EN 438-2, point 21
mm
8
Resistance against scratching
EN 438-2, point 25
Degree
3
Scratch r.
4N
Flexural strength
EN ISO 178
Mpa
100
E-Modulus
EN ISO 178
Mpa
10 000
Tensile strength
EN ISO 527-2
Mpa
60
Susceptibility to cracking
EN 438-2, point 24
5
Thermal properties Dimensional changes during climatic changes, measured at elevated temperatures
EN 438-2, point 17
lenght. %
0,05
cross. %
0,15
Resistance to boiling water
EN 438-2, point 12
%
0,3
Coefficient of thermal expansion
DIN 52328
1/K
20 × 10-6
Thermal conductivity
W/mK
ca. 0,3
Resistance to vapour diffusion
μ
17 200
Surface resistance
DIN 53482
Ohm
109-1011
Resistance to cigarette burns
EN 438-2, point 30
Degree
5 - no visible changes1)
Resistance to hot soucepans
EN 438-2, point 16
Degree
5 - no visible changes, no blisters or cracks2)
MJ/kg
18-20
Level
6-8
Heating value
Optical properties Light fastness
EN 438-2, point 27
1) Slight change in glossy finish, yellow or light brown colours are permitted by EN 438 2) Slight change in glossy finish permitted by EN 438 * These qualities are only suitable for inner lining. The panels should not be exposed to high fluctuations of temperature or moisture. (Recommended range: +15 - +35°C, 30 -70% rel. to air moisture)
Mod. COFORM Rev. 1 del 10/05/2012
Compact Forming Technical Data and Certifications Food onta t suitability Regarding the hygiene regulations concerning materials produced to have contact with foodstiffs (D.M. 4/4/85 - G.U. N° 10 Cee 123, 11/05/1983) it is declared that Compact Forming conforms to the maximum values indicated in Annex IV, Section 2, Paragraph 1. It does not leave free formaldyde in quantities exceeding 0,5 mg/dm2, which is 3 p.p.m., with respect to the real or calculated capacity of the said objet. max 3 p.p.m
for occasional contact
max 0,5 p.p.m
for prolonged occasion
ea tion to ire
lassi i ation
Standard Class 2 Europe EN 13501-1 Euroclass
D-s2, d0
Austria A3800/1
Tr1, Q1
Germany DIN 4102
B2
Class 1 Class 1
CSE RF 1/75/A – 3/77
Home Office Italy
Approbation
T0055A10CD100005
Class M1
CSTB
Home Office France
Certification
89.28703A
Class 1
BSI 476 part. 7: 1987
British Standard Institution UK
Certification
49513
Mod. COFORM Rev. 1 del 10/05/2012
Alucompact Technical Data and Certifications Material properties tested in accordance to EN 438-2 (average value of production control) - Classification CGS Properties
Norms
Unit
Alucompact
Alucompact Arrigo
Alucompact 4, Alucompact 3 Mark1)
Apparent density
DIN 52350/ISO 1183
g/cm3
ca. 1,55
ca. 1,55
ca. 1,65
Thickness (e.g.)
EN 438-2, point 5
mm
10
10
10
15,5
15,5
16,5
450
450
450
Physical data
Weight
kg/m
2
Mechanical properties Resistance against stress abrasion
EN 438-2, point 10
U
Falling ball impact resistance
EN 438-2, point 21
mm
Resistance against scratching
EN 438-2, point 25
degr./ scratch r.
3 4N
3 4N
3 4N
Flexural strength
EN ISO 178
Mpa
200
200
200
E-Modulus
EN ISO 178
Mpa
18 000
18 000
18 000
Tensile strength
EN ISO 527-2
Mpa
Susceptibility to cracking
EN 438-2, point 24
lenght. %
0,15
*
*
cross. %
0,25
*
*
0,3
*
*
Thermal properties Dimensional changes during climatic changes, measured at elevated temperatures
EN 438-2, point 17
Resistance to boiling water
EN 438-2, point 12
%
Coefficient of thermal expansion
DIN 52328
1/K
Thermal conductivity
W/mK
Resistance to vapour diffusion
μ
730 000
Surface resistance
DIN 53482
Ohm
Resistance to cigarette burns
EN 438-2, point 30
Degree
5 - no visible changes2)
5 - no visible changes2)
5 - no visible changes2)
Resistance to hot soucepans
EN 438-2, point 16
Degree
5 - no visible changes, no blisters or cracks3)
5 - no visible changes, no blisters or cracks3)
5 - no visible changes, no blisters or cracks3)
6-8
6-8
6-8
Heating value
MJ/kg
Optical properties Light fastness
EN 438-2, point 27
Level
1) Properties for Alucompact 3 Mark are similar to those of the Alucompact 4 2) Slight change in glossy finish, yellow or light brown colours are permitted by EN 438 3) Slight change in glossy finish permitted by EN 438 * These qualities are only suitable for inner lining. The panels should not be exposed to high fluctuations of temperature or moisture. (Recommended range: +15 - +35°C, 30 -70% rel. to air moisture)
Mod. ALUCOM Rev. 1 del 10/05/2012
Alucompact Technical Data and Certifications e ction to fire cl ssific tion Standard Class 2 Europe EN 13501-1 Euroclass
D-s2, d0
Austria A3800/1
Tr1, Q1
Germany DIN 4102
B2
Mod. ALUCOM Rev. 1 del 10/05/2012
Compact Core Technical Data and Certifications Material properties tested in accordance to EN 438-2 (average value of production control) Properties
Norms
Unit
Value
Apparent density
DIN 52350/ISO 1183
g/cm3
1,55
Thickness (e.g.)
EN 438-2, point 5
mm
10
kg/m2
15,5
450
Physical data
Weight
Mechanical properties Resistance against stress abrasion
EN 438-2, point 10
U
Falling ball impact resistance
EN 438-2, point 21
mm
Resistance against scratching
EN 438-2, point 25
Degree
3
Scratch r.
4N
Flexural strength
EN ISO 178
Mpa
80
E-Modulus
EN ISO 178
Mpa
9000
Tensile strength
EN ISO 527-2
Mpa
60
Susceptibility to cracking
EN 438-2, point 24
4
Thermal properties Dimensional changes during climatic changes, measured at elevated temperatures
EN 438-2, point 17
lenght. %
≤ 0,5
cross. %
≤ 0,8
Resistance to boiling water
EN 438-2, point 12
%
Coefficient of thermal expansion
DIN 52328
1/K
Thermal conductivity
W/mK
Resistance to vapour diffusion
μ
Surface resistance
DIN 53482
Ohm
Resistance to cigarette burns
EN 438-2, point 30
Degree
5
Resistance to hot soucepans
EN 438-2, point 16
Degree
5
Heating value
MJ/kg
Optical properties Light fastness
EN 438-2, point 27
Level
6-8
* These qualities are only suitable for inner lining. The panels should not be exposed to high fluctuations of temperature or moisture. (Recommended range: +15 - +35°C, 30 -70% rel. to air moisture)
Mod. COCORE Rev. 1 del 10/05/2012
Compact Core Technical Data and Certifications ea tion to fire
lassifi ation
Standard Class 2 Europe EN 13501-1 Euroclass
D-s2, d0
Austria A3800/1
Tr1, Q1
Germany DIN 4102
B2
Mod. COCORE Rev. 1 del 10/05/2012
Compact Wood® Technical Data and Certifications Material properties tested in accordance to EN 438-2 (average value of production control) - Classification CGS Properties
Norms
Unit
Value
Apparent density
DIN 52350/ISO 1183
g/cm3
≥ 1,4
Thickness (e.g.)
EN 438-2, point 5
mm
10
kg/m2
14,0
Physical data
Weight
Mechanical properties Resistance against stress abrasion
EN 438-2, point 10
U
450
Falling ball impact resistance
EN 438-2, point 21
mm
8
Resistance against scratching
EN 438-2, point 25
Degree
3
Scratch r.
4N
Flexural strength
EN ISO 178
Mpa
100
E-Modulus
EN ISO 178
Mpa
10 000
Tensile strength
EN ISO 527-2
Mpa
60
Susceptibility to cracking
EN 438-2, point 24
5
Thermal properties Dimensional changes during climatic changes, measured at elevated temperatures
EN 438-2, point 17
lenght. %
0,05
cross. %
0,15
Resistance to boiling water
EN 438-2, point 12
%
0,3
Coefficient of thermal expansion
DIN 52328
1/K
20 × 10-6
Thermal conductivity
W/mK
ca. 0,3
Resistance to vapour diffusion
μ
17 200
Surface resistance
DIN 53482
Ohm
109-1011
Resistance to hot soucepans
EN 438-2, point 16
Degree
5 - no visible changes, no blisters or cracks1)
MJ/kg
18-20
Level
6-8
Heating value
Optical properties Light fastness
EN 438-2, point 27
1) Slight change in glossy finish permitted by EN 438 * These qualities are only suitable for inner lining. The panels should not be exposed to high fluctuations of temperature or moisture. (Recommended range: +15 - +35°C, 30 -70% rel. to air moisture)
Mod. COWOOD Rev. 1 del 10/05/2012
Compact Paint® Technical Data and Certifications Material properties tested in accordance to EN 438-2 (average value of production control) - Classification CGS Properties
Norms
Unit
Value
Apparent density
DIN 52350/ISO 1183
g/cm3
≥ 1,4
Thickness (e.g.)
EN 438-2, point 5
mm
10
kg/m2
14,0
Physical data
Weight
Mechanical properties Resistance against stress abrasion
EN 438-2, point 10
U
450
Falling ball impact resistance
EN 438-2, point 21
mm
8
Resistance against scratching
EN 438-2, point 25
Degree
3
Scratch r.
4N
Flexural strength
EN ISO 178
Mpa
100
E-Modulus
EN ISO 178
Mpa
10 000
Tensile strength
EN ISO 527-2
Mpa
60
Susceptibility to cracking
EN 438-2, point 24
5
Thermal properties Dimensional changes during climatic changes, measured at elevated temperatures
EN 438-2, point 17
lenght. %
0,05
cross. %
0,15
Resistance to boiling water
EN 438-2, point 12
%
0,3
Coefficient of thermal expansion
DIN 52328
1/K
20 × 10-6
Thermal conductivity
W/mK
ca. 0,3
Resistance to vapour diffusion
μ
17 200
Surface resistance
DIN 53482
Ohm
109-1011
Resistance to hot soucepans
EN 438-2, point 16
Degree
5 - no visible changes, no blisters or cracks1)
MJ/kg
18-20
Level
6-8
Heating value
Optical properties Light fastness
EN 438-2, point 27
1) Slight change in glossy finish permitted by EN 438 * These qualities are only suitable for inner lining. The panels should not be exposed to high fluctuations of temperature or moisture. (Recommended range: +15 - +35°C, 30 -70% rel. to air moisture)
Mod. COPAIN Rev. 1 del 10/05/2012
Compact 2002 Technical Data and Certifications Material properties tested in accordance to EN 438-2 (average value of production control) - Classification CGS Properties
Norms
Unit
Value
Apparent density
EN ISO 1183
g/cm3
≥ 1,35
Thickness tolerance
EN 438-2, point 5
mm
5,0 ≤ t < 8,0
± 0,40
8,0 ≤ t < 12,0
± 0,50
12,0 ≤ t < 16,0
± 0,60
16,0 ≤ t < 20,0
± 0,70
Physical data
Mechanical properties Resistance against stress abrasion (wear value)
EN 438-2, point 10
Revolutions
EN 438-2, point 21
mm
≥ 350
Falling ball impact resistance Indentation diameter - 2 ≤ t < 6 mm with 1.4 m drop height Indentation diameter - 6 ≤ t < mm with 1.8 m drop height
h 1400 / d ≤ 10 h 1800 / d ≤ 10
Resistance against scratching
EN 438-2, point 25
Rating
≥ 2 smooth finishes and ≥ 3 textured finishes
Flexural strength
EN ISO 178
Mpa
≥ 80
E-Modulus
EN ISO 178
Mpa
≥ 9000
Susceptibility to cracking
EN 438-2, point 24
Rating
≥4
Thermal properties Dimensional changes during climatic changes, measured at elevated temperatures
EN 438-2, point 17
long. % trasv. %
Resistance to boiling water (thickness increase)
EN 438-2, point 12
%
2 ≤ t < 5 mm1) ≤ 0,40 5 ≤ t < mm1) ≤ 0,30 2 ≤ t < 5 mm1) ≤ 0,80 5 ≤ t < mm1) ≤ 0,60 2 ≤ t < 5 mm
≤6
5 ≤ t mm
≤2
Thermal conductivity
EN 12664
W/mK
0,2 to 0,5
Resistance to water vapour
EN 438-2, point 14
Rating
≥ 3 gloss finishes and ≥ 4 other finishes
Resistance to cigarette burns
EN 438-2, point 30
Rating
≥3
Resistance to dry heat (180°C/ 20 min.)
EN 438-2, point 16
Rating
≥ 3 gloss finishes and ≥ 4 other finishes
EN 438-2, point 27
Grayscale
≥4
Optical properties Light fastness
1) Cumulative dimensional changes
Mod. CO2002 Rev. 1 del 10/05/2012
Compact 2002 Technical Data and Certifications Food onta t Properties
Norms
Unit
Value
Overall migration
EN 1186-3
mg/dm2
3% acetic acid 24 at 40°C
< 10
EN 1186-3
50% ethanol 24 at 40°C
< 10
EN 1186-14
95% ethanol 24 at 40°C
< 10
EN 1186-14
isooctane 24 at 40°C
< 10 < 15
Formaldehyde specific migration
EN 13130-23
mg/kg
3% acetic acid 24 at 40°C
Properties
Norms
Unit
Value
Reaction to fire CGS and ACS types
EN 13501
Class
2 mm ≤ t < 6 mm
D-s1,d0 (metal frame)
t ≥ 6 mm
C-s1,d0 (metal frame)
t ≥ 2,5 mm
D-s2,d0 (wood frame)
t ≥ 2,5 mm
B-s1,d0 (metal frame)
3 mm ≤ t < 6 mm
C-s2,d0 (metal frame and wood frame)
t ≥ 6 mm
B-s1,d0 (metal frame and wood frame)
ea tion to ire
Reaction to fire CGF and ACF types
lassi i ation
EN 13501
Class
Mod. CO2002 Rev. 1 del 10/05/2012